OK Autrod 16.12
GMAW

A stainless ''ER308LSi'' electrode for the GMAW of corrosion-resistant steel containing approximately 19Cr10Ni and austenitic corrosion-resistant steel such as AISI 304, 304L. OK Autrod 16.12 is usually welded with Ar/(1-3%)O2 as the shielding gas.
Welding current, A
DC(+)


ClassificationsApprovalsTypical all weld metal compositionTypical properties all weld metal
SFA/AWS A5.9
ER308LSi
EN 12072
G 19 9 LSi
Werkstoffnummer
~1.4316
DB43.039.01
DNV308L MS (-60°C)
SeprosUNA 485178
UDTDIN 8556
Ü43.039/1
VdTÜV 
C<0,03
Si0,8
Mn1,7
Cr20,2
Ni10,0
Wire composition
Yield stress, MPa
370
Tensile strength, MPa
620
Elongation, %
36
Elongation, %
36
Charpy V
Test temps, °CImpact values, J
+20110
-6090
-19660

Diameter, mm0,60,80,91,01,21,6
Arc voltage, V - 15-24 15-28 15-28 15-29 23-29
Welding current, A - 55-160 65-220 80-240 100-300 230-375
Wire feed, m/min - 4,0-17 3,5-18 4,0-16 3,0-14 5,5-9
Deposition rate kg weld metal/hour - 1,0-4,1 1,1-5,4 1,5-6,0 1,6-7,5 5,2-8,6

 